Heat-Strengthened vs Fully Tempered Glass: A Guide for Facade Designers
Heat-strengthened (HS) glass and fully tempered (toughened) glass are both made by heating annealed float glass and cooling it with air jets, but tempered glass is cooled much faster. The result is that tempered glass is stronger and is classed as a safety glass because it breaks into small, blunt fragments, whereas HS glass is moderately stronger than annealed glass and breaks into large radial pieces. For facades and overhead glazing, HS is often chosen in laminated form because the large fragments interlock and help the laminate stay in place after breakage.
How each type is made
Both products start as annealed float glass that has already been cut to size, edged and drilled. All fabrication must be finished before heat treatment, because neither HS nor tempered glass can be cut, drilled or edge-ground afterwards without breaking. The glass is then heated in a horizontal furnace until it begins to soften.
The difference is in the quench. For fully tempered glass, the hot glass is cooled rapidly by high-pressure air. The surfaces solidify first and the core contracts later, locking the surfaces into high compression balanced by tension in the core. For heat-strengthened glass, the air cooling is gentler and slower, so the surface compression is lower and the internal tension is correspondingly lower.
Strength and breakage behaviour
A rule of thumb used across the industry is that HS glass is roughly twice as strong as annealed glass of the same thickness, and fully tempered glass roughly four to five times as strong. Design strength values come from the applicable standard and the engineer, not from rules of thumb.
Breakage behaviour matters as much as strength:
- Fully tempered glass releases its stored energy on breakage and shatters into many small, relatively blunt pieces. This is why it qualifies as safety glass for human-impact locations.
- Heat-strengthened glass breaks into larger fragments that radiate from the point of fracture, similar to annealed glass but with fewer, longer cracks. It is not a safety glass on its own.
Tempered glass also carries a small risk of spontaneous breakage caused by nickel sulfide inclusions. Because HS glass has lower internal tension, it is generally regarded as far less susceptible to this mechanism, which is one reason facade designers often prefer it where full tempering is not required.
Flatness and optical distortion
Any glass that is heated and transported on rollers can develop roller wave distortion and overall bow. HS and tempered glass share the same furnace process, so both can show distortion; the degree depends on the furnace, the thickness, the size of the pane and the process settings rather than on the product name alone. If reflected appearance is critical, agree flatness limits with the supplier in advance and consider a visual mock-up.
Why HS is often laminated for facades and overhead glazing
When laminated glass breaks, the interlayer holds the fragments together. With two plies of fully tempered glass, both plies can break into small pieces and the laminate may behave like a wet blanket, sagging or falling out of its frame. With HS plies, the larger fragments lock together and give the broken laminate more residual stiffness, so it is more likely to stay in place until it can be replaced.
For this reason, laminated HS is a common choice for overhead glazing, canopies, spandrels and facade units where post-breakage stability is a priority. Where higher strength is needed, for example in point-fixed or highly loaded panels, designers may use laminated tempered or a combination of HS and tempered plies. The final choice belongs to the facade engineer and the local code.
Standards to reference
- EN 1863 covers heat-strengthened soda lime silicate glass in Europe.
- EN 12150 covers thermally toughened (tempered) soda lime silicate safety glass, including the fragmentation test.
- ASTM C1048 covers both heat-strengthened and fully tempered flat glass in the United States, with separate requirements for each.
Comparison at a glance
| Property | Heat-strengthened (HS) | Fully tempered (toughened) |
|---|---|---|
| Cooling rate | Slower, gentler quench | Rapid, high-pressure quench |
| Strength vs annealed | Roughly twice | Roughly four to five times |
| Breakage pattern | Large radial fragments | Small, blunt fragments |
| Safety glass on its own | No | Yes, where it meets the standard |
| Nickel sulfide breakage risk | Generally considered very low | Present; can be reduced by heat soak |
| Post-breakage stability when laminated | Good; fragments interlock | Lower; laminate can sag |
| Cutting or drilling after treatment | Not possible | Not possible |
| Typical standard | EN 1863, ASTM C1048 | EN 12150, ASTM C1048 |
Practical specification checklist
- Confirm the required strength and safety classification with the structural or facade engineer.
- Decide whether the pane must be a safety glass on its own or whether laminating provides the safety performance.
- For overhead or facade units, consider laminated HS for better post-breakage behaviour.
- If tempered glass is used in critical locations, discuss heat-soak testing with the supplier.
- State the applicable standard and the flatness or distortion limits in the specification.
Conclusion
Heat-strengthened and tempered glass are not interchangeable. Tempered glass offers higher strength and safety-glass fragmentation, while HS offers moderate strength, a lower risk of spontaneous breakage and better post-breakage behaviour in laminates. Choosing between them is a question of where the glass is installed, how it is supported and what must happen if it breaks.
Hopson Glass carries out cutting, edging, drilling, tempering and laminating in-house. Send your drawings and glass make-up to our team for a quotation on heat-strengthened, tempered or laminated panels.