Heat Soak Testing and Nickel Sulfide (NiS) Spontaneous Breakage Explained

Hopson Glass technical team ·

Summary: Nickel sulfide (NiS) inclusions in float glass can cause fully tempered glass to break without any external load, sometimes long after installation. A heat-soak test deliberately accelerates this process in a controlled oven so that most affected panes break in the factory, which reduces but does not eliminate the risk on site.

Spontaneous breakage of tempered (toughened) glass is most often caused by tiny nickel sulfide (NiS) inclusions trapped in the glass during float manufacture. After tempering, these inclusions can slowly expand and crack the pane with no impact or load. A heat-soak test exposes tempered panes to elevated temperature for a set period so that panes containing critical inclusions are more likely to break in the factory rather than on the building. It reduces the risk significantly but cannot remove it entirely.

What nickel sulfide inclusions are

Nickel sulfide inclusions are microscopic particles that can form when traces of nickel come into contact with sulfur in the glass melt. Sources of nickel contamination include raw materials, process equipment and stainless steel fragments. The inclusions are generally too small to be seen by eye or detected reliably in routine inspection of finished glass.

At the high temperatures used in glass making and tempering, nickel sulfide exists in a high-temperature crystal form. When the glass cools slowly, the inclusion has time to change to its low-temperature form. When the glass is cooled very quickly, as in tempering, the high-temperature form is effectively frozen in place. Over time, at normal service temperatures, it gradually transforms back, and this phase change is accompanied by a small increase in volume.

Why tempered glass is affected, but not HS or annealed glass

Tempered glass has a core under high tensile stress, balanced by compressed surfaces. If an expanding inclusion sits in that tensile core, the local stress it creates can be enough to start a crack, and the stored energy in the pane then drives the crack across the whole panel. The fracture origin often shows a characteristic pattern of two adjoining fragments that look like a butterfly, with the inclusion at the centre.

Annealed glass has no significant built-in tension and is cooled slowly, so inclusions have time to transform during manufacture. Heat-strengthened glass is cooled more gently and has much lower central tension, so it is generally regarded as far less susceptible. This is one reason designers use HS glass where full tempering is not required.

How a heat-soak test works

Heat soaking is carried out after tempering, as a separate process:

  1. Tempered panes are loaded into a dedicated oven on racks, spaced so that air can circulate and broken pieces do not damage neighbouring panes.
  2. The oven is heated until the glass reaches a defined holding temperature, monitored with thermocouples attached to the glass.
  3. The glass is held at that temperature for a defined period. The heat accelerates the phase change of any nickel sulfide inclusions.
  4. The oven is cooled in a controlled way, and the surviving panes are inspected, recorded and labelled.

Panes containing critical inclusions are more likely to break during this cycle, so they are removed before delivery. Because the glass must survive temperature exposure on the rack, heat soaking must be done before laminating or assembling into insulated glass units.

In Europe, heat-soaked thermally toughened safety glass is defined by EN 14179, which sets out the process and the factory production control requirements. Other regions have their own approaches, and some project specifications write their own heat-soak clauses.

What heat soaking cannot do

Heat soaking is a risk-reduction measure, not a guarantee. Not every critical inclusion will cause breakage during the test, and the process depends on correct oven control, temperature uniformity and record keeping. Specifiers should therefore treat heat-soaked glass as lower-risk rather than risk-free, and should still design critical glazing so that a breakage does not cause a dangerous fall of glass.

When to specify heat soaking

Heat soaking adds cost and lead time, so it is normally reserved for locations where a spontaneous breakage would be dangerous, disruptive or very expensive to repair:

  • Facade and curtain-wall glazing, particularly at height or above public areas.
  • Overhead glazing, canopies and skylights where tempered plies are used.
  • Glass balustrades and barriers, especially where tempered plies are used in laminates.
  • Structural glass fins and point-fixed glass.
  • Large or hard-to-access panes where replacement requires cranes or access equipment.

Alternatives or complements include using heat-strengthened glass where its strength is sufficient, and laminating so that a broken pane is retained by the interlayer.

Specification and procurement checklist

ItemWhat to ask or specify
StandardName the standard required, for example EN 14179, or the project heat-soak clause
CapabilityAsk your supplier whether heat soaking is done in-house or by a partner
Process recordsRequest oven cycle records and temperature logs for each batch
MarkingConfirm how heat-soaked panes are marked or labelled
SequenceConfirm heat soaking is completed before laminating or IGU assembly
Lead timeAllow for the extra process step in the programme
DesignConsider HS glass or laminated make-ups to manage residual risk

Conclusion

Nickel sulfide breakage is a known characteristic of fully tempered glass rather than a manufacturing defect in the usual sense. Heat soaking is the established way to reduce the risk, and it is worth specifying wherever a spontaneous breakage would put people or the building at risk. Combine it with sensible glass selection and laminating for critical glazing.